Precision ceramic materials combine nanoscale powders with advanced sintering processes to provide excellent high-temperature resistance, high hardness and strong corrosion resistance. They outperform traditional materials in extreme environments and support precise, complex custom structures for varied applications. Their biocompatibility, electrical insulation and non-magnetic properties help improve equipment stability and durability, offering innovative material solutions for precision industries.

Material property comparison

氧化铝增韧氧化锆
氧化锆增韧氧化铝
红宝石
蓝宝石
氮化铝
氮化硅
碳化硅

图表数值为典型参考值或范围中位值,仅用于材料初步选型。实际性能会因材料牌号、纯度、成型方式、烧结工艺和测试标准而变化。

性能 单位 材料 材料 材料 材料 材料 材料
氧化铝 氧化锆 宝石 氮化铝 氮化硅 碳化硅
96% 99% 99.9% 99.99% 钇稳定氧化锆 氧化铝增韧氧化锆 氧化锆增韧氧化铝 蓝锆 黑锆 红宝石 蓝宝石
颜色 / 白色白色象牙黄象牙黄白色白色白色蓝色黑色红色白色白色黑色黑色
密度 g/cm3 ≥3.743.93.93.9≥6.05.65.6≥6.0≥6.03.953.953.283.23.15
吸水率 % 00000000000000
抗弯强度 Mpa ≥300300350380800-1400800-1400800-14001000-14001000-1400800-1000800-1000350610300
维氏硬度 Gpa ≥1515181214141414141414913.920
断裂韧性 MPa m1/2 33444664455454
热导率 W/mK ≥202032281.5221.51.525251802345
热膨胀系数 1*10-6 mm/c 6.67.27.37.39.810109.89.88.58.54.52.64
耐热温度 ℃ 16001600160016002000120012002000200019001900150015001500
抗热震性 △T 200-300℃300-500℃300-600℃300-600℃400-1000℃400-800℃300-700℃400-1000℃400-1000℃200-300℃200-300℃200-300℃800-1000℃700-900℃
介电常数 / 9.4±0.399.81026101026269.39.38.68.69.4
介电损耗 *10-4 ≤32220.010.010.010.010.0111111
体积电阻率 Ω.cm >10141014101410151012--101210121014101410111014106
击穿电压 KV/mm >1212>12>12588551010121212

以上数据为典型参考值,仅用于材料初步选型。实际性能会因材料牌号、纯度、成型方式、烧结工艺和测试标准而变化。如需特定牌号数据,请以技术确认文件为准。